Our Materials
Evazote® VA35 Foam
Evazote® VA35 is designed for applications where low weight, toughness and long-term performance are essential. Its closed-cell structure provides low water absorption and excellent tear resistance, making it suitable for demanding industrial, sports and leisure applications.
Characteristics of Evazote ® VA35
- Lightweight
- Superior softness
- Excellent resilience
- Low water absorption
- High-impact absorption
- Long-lasting performance
Key Properties of Evazote® VA35 Foam
- Density : 35 kg/m
- Cell Size : 0.5mm
- Shape Recovery : 10%
- Stretchability : 145 kPa
- Shore Hardness : 50 OO
- Compressibility : 52 kPa
- Strength : 545 kPa
- Durability : 1970 N/m
- Max Operating Temp : 70°C
- Water absorption : <1%
Foams manufactured in a selection of colours
Black
White
Red
Blue
*Other colours may be available on request. All colours are subject to foam type, minimum order quantity, and suitable masterbatch availability.
Typical performance data for Evazote®VA35 Foam
| Property | Value | Test Method |
|---|---|---|
| Apparent density | 35 kg/m | BS EN ISO 7214:2012 |
| Cell size | 0.5mm | Internal |
| Shore hardness | 50 OO | BS EN ISO 868:2003 |
| Water absorption | <1% | ISO 2896:2001 Ed3. |
| Property | Condition | Value | Test Method |
|---|---|---|---|
| Compression stress | 25% Compression | 52 kPa | BS EN ISO 7214:2012 |
| Compression stress | 50% Compression | 118 kPa | BS EN ISO 7214:2012 |
| Tensile strength | Standard | 545 kPa | BS EN ISO 7214:2012 |
| Tensile elongation | Standard | 145% | BS EN ISO 7214:2012 |
| Tear strength | Method B | 1970 N/m | BS EN ISO 8067:2008 |
| Property | Condition | Value | Test Method |
|---|---|---|---|
| Compression set | 25% comp, 22hr, 23oC, ½ hr recovery | 10% | BS EN ISO 7214:2012 |
| Compression set | 50% comp, 22hr, 23oC, 24 hr recovery | 3% | BS EN ISO 7214:2012 |